Delayed Cracking of Advanced High Strength Steel Solutions

2018-10-25 13:48:00
LUQIMENG
Original
2444

Mentor: Dean Kanelos - - Nucor Steel
Co- - Principal Investigator: Eric Batt - ArcelorMittal
Co- - Principal Investigator: Curt Horvath – General Motors Company

Project Manager: Jonathan Smith, Auto/Steel Partnership


A/SP Team Members:
J. Bickham – ArcelorMittal
J. Cole – Ford Motor Company
R. J. Comstock – AK Steel
J. J. Coryell – General Motors Company
C. Matthew Enloe – General Motors Company
J. J. Fitzpatrick - ArcleorMittal
M. P. Hammerl – AK Steel
M. M. Huang – ArcelorMittal
P. Makrygiannis – AK Steel
A. D. Pearson – General Motors
R. Radzilowski – AK Steel
N. Ramisetti – ArcelorMittal
D. S. Ruhno – Ford Motor Company
J. Singh – FCA Group
P. Som -ArcleorMittal
J. Stachowski - Nucor
A. Thompson - Nucor
Y. Wang – AK Steel
S. Wolf - ArcelorMittal

W. Wu – AK Steel


? To develop a test method for ranking the relative susceptibility of zinc coated advanced high strength steels (AHSS) and ultra-high strength steels (UHSS) to hydrogen assisted cracking.
? To avoid the most common concerns with existing tests:
? Artificial “charging” with hydrogen concentrations far above what
would be expected in automotive environment
? Development of a test that is not relevant to thin sheet steels
? Development of a test that is complicated and/or requires R&D type
of equipment


? To expand on the previous work done by the A/SP STHT which resulted in a draft procedure for determining the relative susceptibility of bare AHSS/UHSS
? To develop a representative test for zinc coated steels

? A test that is relatively easy to run and adapted for new grade validation
? A test that can be modified for specific OEM pass/fail criteria.
? A test that is applicable to sheet steel with or without additional manufacturing (coating, welding, etc.) or in-service corrosion inputs

Note: : t It s is commonly thought that the risk for hydrogen assisted cracking cannot be completely eliminated (in all potential processes/environments) unless tensile strengths are restricted below 800 MPa


? A bend test consisting of samples pre-strained to >/=70% of their yield strength shows promise for evaluating hydrogen susceptibility
? Some materials/microstructure combinations with high tensile strengths have been shown as susceptible to hydrogen assisted cracking when exposed to test conditions
? Hydrogen related cracks occur very early in the test.

? Multiple test labs have seen similar results when susceptible materials are evaluated to the new test method.
? The A/SP Sheet Steel Harmonization Task Force has developed a draft test method for testing uncoated steels.
? When testing zinc coated steels with 0.1N HCl, the generation of hydrogen during dissolution can lead to premature fracture.


? Samples are strain-gauged and bent to the desired stress levels
? Fixtured samples are immersed in 0.1 N hydrochloric acid


Observation:
Susceptible materials at high
strains, immersed in 0.1N HCl,
exhibit large cracks after relatively
short exposures to the acid solution

? Goal: Work with AET Integration, Inc. to determine adaptations needed to current draft procedure to allow testing of grades with zinc coatings
? Comparison of different concentrations of hydrogen source (NH 4 SCN) to previously studied HCl.
? Testing of dual phase, fully martensitic and press hardened grades.



? Use of NH 4 SCN resulted in a significantly lower attack on the coatings than the previously used HCl
? The lower rate of attack on the zinc coatings in the NH 4 SCN solutions (ie low mass loss), likely resulted in low/little hydrogen evolution and lower amounts of hydrogen absorption


? The use of a NH 4 SCN solution appeared to greatly reduce or eliminate hydrogen evolution of zinc coated AHSS’s

? The use of NH 4 SCN does show promise as an alternative test solution to .1N HCL, however, lower concentrations than those tested need to be evaluated for use on zinc coated substrate

? Investigate lower concentrations of NH 4 SCN
? Investigate techniques for coating removal
? Follow with acid immersion bend test
? Test coated substrate to SEP1970 – Tensile Specimen with Punched Hole
? Others?





Write a Comment
Two multiply Two =
Comment will be posted after it is reviewed.
QR Code
主站蜘蛛池模板: 十八禁视频在线观看免费无码无遮挡骂过 | 久久精品亚洲精品无码白云tv| 97久久天天综合色天天综合色hd| 日日日日做夜夜夜夜做无码| 国产一区二区内射最近更新| 亚洲欧美成αⅴ人在线观看| 国产成人av性色在线影院| 精品国产污污免费网站入口| 国产人成无码视频在线1000| 亚洲人成绝费网站色www| 亚洲v欧美v国产v在线观看| 国产精品无码专区| 国产精品乱码人妻一区二区三区| 国产精品爱久久久久久久电影蜜臀 | 熟妇人妻久久中文字幕| 在线播放国产精品三级| 2020精品国产午夜福利在线观看| 精品一区二区三区东京热| 性生交大片免费看| 日本极品少妇videossexhd| 亚洲乱码一区二三四区ava | 国产成网站18禁止久久影院| 天堂中文在线资源库用| 男女一边摸一边做爽爽的免费阅读 | 亚洲综合av永久无码精品一区二区| 国产美女无遮挡裸色视频| 牲欲强的熟妇农村老妇女| 亚洲国产精品一区二区成人片国内 | 国产成人午夜福利高清在线观看 | 久久久久av无码免费网| 久久亚洲人成网站| 国产男人的天堂在线视频| 亚洲人成电影在线观看青青| 欧美精品黑人粗大| 亚洲色无码专区一区| 久久综合网欧美色妞网| 人人妻人人澡人人爽久久av| 丰满的岳久久乱| 欧美日韩国产综合新一区| 欧美日韩免费专区在线| 无码手机线免费观看|